Packaging for Long Sea Routes: What Actually Prevents Damage

Nov 13, 2026

Leave a message

Packaging for Long Sea Routes: What Actually Prevents Damage

A container crossing the Indian Ocean passes through four or five condensation cycles. Steel that was dry when it was loaded can arrive with white rust, stained plate edges or deformed coil wraps. None of it is caused by the steel, and almost all of it is preventable at packing.

The damage mechanisms

Container rain. Warm humid air inside the container condenses on the steel as it cools at night, then evaporates and re-condenses. The cycle repeats for the whole voyage, and the water ends up on the top surface and in the coil wrap.

Salt mist in transit. On deck stow or in a transhipment port, airborne chlorides settle on any exposed surface and start pitting.

Mechanical damage. Straps that are too few, dunnage that is too thin, and bundles that rub against each other for three weeks.

What works, in order of cost effectiveness

  1. Keep the wrap sealed. VCI film is only effective while it is intact. One cut, and the protection is gone for the whole coil.
  2. Desiccant in the right quantity. Roughly 1 kg of desiccant per 10 m³ of container volume for a 30 day voyage, hung high so the condensate runs away from it, not through it.
  3. Container lining or desiccant blankets. A liner reduces the condensation that forms on the ceiling and drips onto the cargo.
  4. Edge protectors and corner boards on every bundle, so straps bear on cardboard or plastic, not on the steel edge.
  5. Timber dunnage between layers and at the door end, so nothing shifts when the doors open.
  6. Oil or VCI on machined or bright surfaces, applied before packing, not after arrival.

What not to bother with

  • Thicker plastic wrap on its own - it traps condensation as effectively as it keeps rain out
  • Desiccant left in a torn bag, or placed on the floor where the water collects
  • Silica gel sachets sized for a carton of electronics, in a 40HQ of steel

A packing spec that survives the route

For hot and humid destinations we specify: VCI film on cold rolled and coated coils, edge protectors on all bundles, timber dunnage at floor and door, straps at 1.5 m centres, desiccant at the calculated quantity, and shrink wrap on palletised goods. For plate, interleaved dunnage and corner protection matter more than film.

Photograph the packing before the doors close. A photo of the stow is the cheapest evidence there is if a claim is raised.

What we do

  • Packing specified for the route and the season, not a default export standard
  • Desiccant quantity calculated from container volume and transit time
  • Pre-shipment photos of the stow, the straps and the seals
  • Receiving note with the documents, so the person at destination knows what to check first

Tell us the destination and the transit time. We will propose the packing that fits that route, and show it on the quotation so there is no assumption on either side.

Related: Container loading, Steel coil storage and handling, Galvanized coil

Frequently asked questions

What causes container rain?

Warm humid air inside the container condenses on cooler steel overnight, then evaporates and re-condenses throughout the voyage.

How much desiccant does a 40HQ need?

Roughly 1 kg per 10 m3 of container volume for a 30 day voyage, hung high so condensate does not run through it.

Does thicker plastic wrap help?

No. Without ventilation it traps condensation as effectively as it keeps rain out.